Platinum Iridium Piping issues
- YanQing Tang
- Topic Author
- Offline
- Fresh Boarder
Less More
11 years 6 months ago - 11 years 6 months ago #2558 by YanQing Tang
Platinum Iridium Piping issues was created by YanQing Tang
We have recently encountered piping issues on our Platinum Iridium rods. there's no process change, what are the possible root causes?
thanks for the help.
Mandy
thanks for the help.
Mandy
Attachment 350218-lot-286043-414166receved-5-15-13.JPG not found
Attachments:
Last edit: 11 years 6 months ago by YanQing Tang.
Please Log in to join the conversation.
- Peter J Stewart-Hay
- Offline
- Moderator
Less More
- Posts: 126
- Thank you received: 21
11 years 5 months ago - 11 years 5 months ago #2559 by Peter J Stewart-Hay
Regards,
Peter J. Stewart-Hay Principal
Stewart-Hay Associates
www.Stewart-Hay.com
This email address is being protected from spambots. You need JavaScript enabled to view it.
Replied by Peter J Stewart-Hay on topic Re: Platinum Iridium Piping issues
Hello;
This seems to me as if it is a central burst defect (AKA a Cup-cone fracture or chevroning.) Often this is the result of putting a die in backwards in a drawing machine.
Please see www.metalforming-inc.com/publications/bo.../chapter_3/3-5-5.pdf
This seems to me as if it is a central burst defect (AKA a Cup-cone fracture or chevroning.) Often this is the result of putting a die in backwards in a drawing machine.
Please see www.metalforming-inc.com/publications/bo.../chapter_3/3-5-5.pdf
Regards,
Peter J. Stewart-Hay Principal
Stewart-Hay Associates
www.Stewart-Hay.com
This email address is being protected from spambots. You need JavaScript enabled to view it.
Last edit: 11 years 5 months ago by Peter J Stewart-Hay.
The following user(s) said Thank You: YanQing Tang
Please Log in to join the conversation.
- YanQing Tang
- Topic Author
- Offline
- Fresh Boarder
Less More
- Posts: 4
- Thank you received: 0
11 years 5 months ago #2591 by YanQing Tang
Replied by YanQing Tang on topic Re: Platinum Iridium Piping issues
Any recommneded equipments where we can detect piping without breaking up the wires at this fine size(0.098")? We use Ultrasound, but at wire size of 0.5".
Please Log in to join the conversation.
- Peter J Stewart-Hay
- Offline
- Moderator
Less More
- Posts: 126
- Thank you received: 21
11 years 5 months ago - 11 years 5 months ago #2594 by Peter J Stewart-Hay
Regards,
Peter J. Stewart-Hay Principal
Stewart-Hay Associates
www.Stewart-Hay.com
This email address is being protected from spambots. You need JavaScript enabled to view it.
Replied by Peter J Stewart-Hay on topic Re: Platinum Iridium Piping issues
I do not know of any instrumentation that can see inside the wire at diameters less than 1/10 inches.
Fortunately central burst failures are very rare in common metal (copper and aluminum) drawing practice. One of the indications you get on the surface of the conductor is chevroning which is often called "Crows Feet" which actually describes what the chevrons look like. Please see this web site for more information:
books.google.ca/books?id=YXp6zao0HqgC&pg...%20in%20wire&f=false
Thus there may be chevrons on the surface of your wire when central bursting occurs. The chevrons point in the direction that the wire was drawn. Thus you may be able to see the chevrons on the surface of the wire. The other indication of central bursting is that; "If you bend a piece of central burst wire between your fingers, it usually breaks like a dry twig."
Presumably central burst failures are very rare for you as well. If this is true, I very much doubt that you really need on-line scanning instruments. ( I of course know nothing of the drawing process and drawing failures in platinum Iridium wire but I am assuming that the wire drawing problems are similar. I am also assuming that there was no internal defects in the platinum Iridium to start with Before it was drawn).
Here are the typical reasons for chevron formation: (WAI Nonferrous Handbook Volume 2: Bare Wire Processing)
Fortunately central burst failures are very rare in common metal (copper and aluminum) drawing practice. One of the indications you get on the surface of the conductor is chevroning which is often called "Crows Feet" which actually describes what the chevrons look like. Please see this web site for more information:
books.google.ca/books?id=YXp6zao0HqgC&pg...%20in%20wire&f=false
Thus there may be chevrons on the surface of your wire when central bursting occurs. The chevrons point in the direction that the wire was drawn. Thus you may be able to see the chevrons on the surface of the wire. The other indication of central bursting is that; "If you bend a piece of central burst wire between your fingers, it usually breaks like a dry twig."
Presumably central burst failures are very rare for you as well. If this is true, I very much doubt that you really need on-line scanning instruments. ( I of course know nothing of the drawing process and drawing failures in platinum Iridium wire but I am assuming that the wire drawing problems are similar. I am also assuming that there was no internal defects in the platinum Iridium to start with Before it was drawn).
Here are the typical reasons for chevron formation: (WAI Nonferrous Handbook Volume 2: Bare Wire Processing)
- - Misaligned wire entering a drawing die.
- - An improper die contour such as;: badly blended angles inside the die, too short or no bearing on the die, wrong entrance or reduction angle (Such as putting a die in backwards.)
- - Improper or insufficient lubrication.
Regards,
Peter J. Stewart-Hay Principal
Stewart-Hay Associates
www.Stewart-Hay.com
This email address is being protected from spambots. You need JavaScript enabled to view it.
Last edit: 11 years 5 months ago by Peter J Stewart-Hay.
The following user(s) said Thank You: YanQing Tang
Please Log in to join the conversation.